             Conditions for injection molding of cosmetic packaging:
               1.  multi-cavity injection molding, product requires balance;
               2. new transparent materials such as PETG and PCTG, with a wall
                   thickness of 3-10mm;
               3. the price of new materials is high, and the appearance of injection
                   products is mostly high-gloss or transparent.

     Key points of molding:
             1. multi-cavity injection design should be balanced.
             2. high pressure and low speed hot runner without leakage.
             3. full hot runner valve injection be adopted .

Application case

                 Zhenxiong's technology helps package manufacturers achieve maximum output by
          shorten processes and minimizing material loss.We provide economical and reliable
          results, as well as part design, material, mold design, machine, runner, flow control
          system and auxiliary equipment combination to meet your requirements.The most
          demanding production process is thin-walled packaging. Zhenxiong has mastered
          a lot of relevant technologies, which can help you produce thin-walled packaging
          and achieve the highest output.
                Zhenxiong's products ensure the efficiency, precision and repeatability required by
          the packaging industry.Our comprehensive service and support can provide you
          with everything you need, including customization when necessary, first-class
          machining, efficiency evaluation and improvement suggestions.












Causes of product imbalance injection
 1. The temperature of the manifold or the heatcoil is unbalanced.
     The manifold heatcoil is arranged with the round heating pipe coated
     with copper method, its design using each group of independent  
     heating partition, temperature independent controlled.
2. Irregular distribution and balance scheme of manifold .
    Irregular distribution through the flow analysis of zhenxiong, the
    diameter of the runner and the size of the gate are adjusted to
    achieve the best flow balance.
3. The diameter of nozzle and local hot spots lead to temperature
    imbalance.
   The nozzle runner diameter is consistent and the temperature design
   is balanced, as shown in the figure on the right.








Zhenxiong nozzle is polished by the runner polishing machine after processing with the gun drill, and the heating circle is inlaid with copper sleeve to ensure the temperature balance relying on the high heat conduction of the copper sleeve.Independent thermocouple + with double temperature sensor, HOTSET quality, stable quality, easy maintenance.
 

Solution

     》Reasons for system leakage.
    ■ 
Zhenxiong manifold is inserts and polished by the runner polishing machine
         Along with Hot fit application (interference fit) without leakage .


         Leakage of nozzle sealing
    
■ Zhenxiong has strict testing training and requirements for all the installation
        personnel. Only when all the dimensions are processed accurately according
        to the drawings can they be  installed to ensure no leakage.

         Nozzle and manifold matching surface leakage.
    
■ zhenxiong design has avoided possible machining errors, as shown in the
        right figure
    
■ Zhenxiong focuses on engineering materials and high glass fiber products
        Imported steel, specially treated, more wear - resistant and corrosion - resistant
    
■ Zhenxiong nozzles are made of imported steel with special treatment,
        effectively ensuring the life of products. The quality of hot runner products is
        designed with 10 years' service life, and  the design life of products with fiber
        added within 15% is designed with 2 million times of mold.


 





  》Zhenxiong focuses on engineering material and high fiber  products
      
Imported steel, specially treated, more wear - resistant and corrosion -resistant
      Zhenxiong nozzles are made of imported steel with special treatment, effectively ensuring the life of products. The quality of hot runner
      products is designed with 10 years' service life, and the design life of products with fiber added within 15% is designed with 2 million times of mold.





    Reasons for products yellowing ,black coating.
   
■ Dead angle existed in nozzle outlet .
        Zhenxiong has professional MTO patent for molding transparent/color  changing  products nozzle.This type of nozzle
        has no dead angle, fast  color change  and small pressure loss.
   
■ There is a dead angle at the corner of the manifold. The plug at the 
         junction angle of the runner adopts smooth transition, and the special 
         position adopts mosaic structure to ensure the junction angle is smooth.
   
■ The plastic material stays in the runner too long.
         See attached page for detailed calculation of plastic injection volume and
         residence time



 














Nozzle temperature difference accuracy
   The internal temperature error of zhenxiong nozzle is no more than 10 degrees.
     
    product standard

    1. 90% of the products are standardized and 90% are in
         sufficient inventory.
        Standardized production ensures the consistency of quality.
    2. Material import
        Nozzles are made of ASSAB imported materials, and the
        processing technology is strictly controlled to ensure the 
        interchangeability of     
       nozzles  effectively.
    3 .Process standard
        The heating coil winding method has been tested strictly, the winding 
        process is standardized, and high quality is required to ensure stable 
        quality.
 






  》Causes of wire drawing drooling of gate.
       There is no reasonable cooling at the tip of the nozzle.
       Reasonable cooling water line should be designed near the nozzle gate to increase
       cooling Water line can avoid problems such as wire drawing and drooling caused by
       heat accumulation at the gate 
       The nozzle selection is unreasonable
       Zhenxiong nozzle is a special structure without nozzle core, without drawing and
       drooling. Valve type nozzle is recommended for drawing caused by extreme injection
       molding condition .
       The temperature of nozzle is not stable and the long-term production stability is poor.
       Zhenxiong heating accessories are imported , see the attached page


















   》Causes for valve needle stuck:
         1. The valve needle is too long with the needle brush.
         The matching length between the guide brush and the valve needle of zhenxiong
         is shorter than other companies,which get less needle stuck.
     2. Improper fitting tolerance between valve needle and needle brushing.
         The matching tolerance between the guide brush and the valve needle of Zhenxiong
         is customized according to the fiber adding material, and it has been tested and verified
         repeatedly to ensure no leakage and needle stuck.
     3. Processing error leads to unqualified or unstable quality.


























.
Market solutions
Mobile
Precision Electronics
Liquid Silicon Rubber
Television
Household Appliances
Office Products
Optical Illumination
Automobile
Medical Packaging
Food Packaging
Cosmetic packaging
Products
Hot runner system
Nozzle
Manifold
Heating plate
Insulation board
Temperature Controller
Heating elements
Heatcoil
Thermocouple
Timing controller
Technical Support
Contact support Dept.
Technical training
Free mold flow analysis
Service
Pre-sales proces
After sales process
Product warranty details
Product specification
Hot runner data
Cold runner data
Remote technical data
Online Ordering
Online mall
Q&A
Production of consulting
Evaluation
Improvement
Planning
Company Brand
About Us
Development
CEO speech
Reasons to choose us
Working conditions
Development planning
Join Us
FAQ
Contact US
Servcie Technical Support
Training
Local service network
Online custom hot runner
Contact Information
Shenzhen ZhenXiong Hot Runner Technology co. LTD © 2019     备案号/许可证编号:粤ICP备12037482号
*This website webpage material small part of source Internet, if infringement, please inform us, we will be deleted within 24 hours. The pictures on the website of our company are taken by our products*
c
o
n
t
a
c
t
u
s